Izixazululo Nezinyathelo Zokuvimbela I-Aluminium Die Casting 10 Amaphutha Amakhulu
Amamaki Wokugeleza Namaphethini
Ukuhlola ukubukeka: Kunemivimbo ebusweni bokusakaza ehambisana nokuhamba kokugeleza kwensimbi encibilikisiwe, futhi kusobala ukuthi kunemigqa engeyona eyokuqondisa ehlukile kumatrix ensimbi ngombala, futhi awukho umkhuba wentuthuko.
1. Izimbangela zamamaki okugeleza zimi kanje:
- Izinga lokushisa lesikhunta liphansi kakhulu
- Idizayini embi yomgijimi nesimo esibi esangweni langaphakathi
- Izinga lokushisa eliphansi kakhulu
- Ijubane lokugcwalisa okuphansi nesikhathi esifushane sokugcwalisa
- Isistimu yokubamba engenangqondo
- Ukukhishwa kabi
- Isifutho esingenangqondo
2. Imbangela yephethini ngopende omningi kakhulu emgodini noma ikhwalithi yepende empofu. Izixazululo nezindlela zokuvimbela zimi kanje:
- Lungisa indawo enqamulelayo noma isikhundla somgijimi wangaphakathi
- Khulisa lokushisa isikhunta
- Lungisa ijubane nengcindezi yomgijimi wangaphakathi
- Ukukhetha okufanele upende nokulungiswa kwesilinganiso
Izimpiko Zenwele Ezenziwe Inethi (Ufudu Oluqhekekile)
Ukuhlolwa kokubukeka: Ubuso bezingxenye zokufa zinezici ezifanayo eziphakanyisiwe noma ezicindezelekile njengezinwele ezinjenge-net, ezizokwanda futhi zinwebe njengoba inani lokuphonsa abafayo lenyuka.
Izizathu zingokulandelayo:
- 1) Kukhona imifantu ebusweni bomgodi wokuphonsa
- 2) Preheating engalingani of die ekubunjweni isikhunta
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Isikhunta sokufa kufanele sithuthukiswe njalo noma ngemuva kwenombolo ethile yokufa ukuze kuqedwe ukucindezeleka emgodini
- 2) Uma kuqhamuke uqhekeko lofudu ebusweni bomgodi, indawo yokubumba kufanele ipholishwe ukususa ungqimba lokuqhekeka
- 3) Preheat isikhunta ngokulinganayo
Isithiyo Esibandayo
Ukubukeka kokuhlola: Ubuso bokuphonsa okufayo kunemigqa eqondile, engajwayelekile, futhi ecwilayo (yomabili engenayo nengangeniyo). Umumo mncane futhi mude, kwesinye isikhathi umkhawulo wokuhlangana ubushelelezi, futhi kukhona nokwenzeka kokunqanyulwa ngaphansi kwesenzo samandla angaphandle.
Izizathu zingokulandelayo:
- 1) Imifudlana emibili yensimbi ixhunywe komunye nomunye, kepha ayihlanganisiwe ngokuphelele futhi akukho okuhlanganisiwe phakathi, namandla okubopha emifudlana emibili yensimbi abuthakathaka kakhulu.
- 2) Izinga lokushisa lokuthululela noma lokushisa lokufa liphansi kakhulu
- 3) Isimo somgijimi asilungile noma indlela yokugeleza yinde kakhulu
- 4) Ijubane lokugcwalisa okuphansi
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Khulisa kahle izinga lokushisa elithelekayo
- 2) Thuthukisa isilinganiso somjovo, cindezela isikhathi sokugcwalisa futhi wandise isivinini somjovo
- 3) Thuthukisa izimo zokukhipha nokugcwalisa
I-Shrinkage (Dents)
Ukuhlola okubonakalayo: Kunamazinyo abushelelezi (njengamadiski) ebusweni obukhulu kakhulu bokusakaza okufa.
Izizathu zingokulandelayo:
- 1) Kubangelwa ukuncipha: Idizayini engalungile yezingxenye zokufa ezifa ngobukhulu obukhulu kakhulu odongeni ubukhulu / indawo engalungile yomgijimi / isilinganiso sokujova siphansi, isikhathi sokubamba ingcindezi sifushane, futhi izinga lokushisa lendawo lokufa kwesikhunta liphakeme kakhulu
- 2) Idizayini yokupholisa engenangqondo
- 3) Ukuvula isikhunta kusenesikhathi
- I-4) Izinga lokushisa eliphakeme kakhulu
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Ubukhulu bodonga kufanele bufane
- 2) Ushintsho lokujiya kufanele lwenziwe lula
- 3) Khetha ngokufanele indawo yokungenisa i-alloy liquid futhi wandise indawo enqamula umgijimi wangaphakathi
- 4) Khulisa ingcindezi yomjovo futhi wandise isikhathi sokubamba ingcindezi
- I-5) Nciphisa ngokufanele ukushisa okuthululelayo nokushisa okufayo
- 6) Ngokwengxenye kuphole ukushisa okuphezulu kwasendaweni
- 7) Thuthukisa izimo zokuchichima
Imprint
Ukuhlola okubonakalayo: iminonjana eshiywe ngokuxhumana phakathi kobuso bokusakaza kanye nobuso bomgodi wokuphonsa noma amamaki esinyathelo avela ebusweni bokusakaza.
Izizathu zingokulandelayo:
1. Kubangelwa izingxenye ze-ejector
- 1) Ubuso bokugcina benduku ye-ejector bugqokiwe
- 2) Ubude bokulungiswa kwenduku ye-ejector abuhambisani
- I-3) Ingxenye yokusiceba yomgodi wokufa ayihambelani kahle nezinye izingxenye
2. Kubangelwa ukusikwa noma izingxenye ezihambayo
- 1) Ingxenye ye-inlay ivulekile
- 2) Izingxenye ezikhululekile noma ezigugile ezihambayo
- 3) Ubuso obusodongeni bokuphonsa benziwa ukufakwa okuhlukaniswe yisikhunta esigudlukayo nesilungisiwe
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Ubude benduku ye-ejector kufanele buguqulwe buye endaweni efanele
- 2) Bopha ukufaka noma ezinye izingxenye ezihambayo
- 3) Susa amakhona abukhali lapho udizayina, bese ulungisa ukulingana igebe
- 4) Thuthukisa isakhiwo castings ukuqeda egxiliwe inlay ifomu isikhunta die-ekubunjweni futhi sithuthukise isakhiwo die-ekubunjweni isikhunta
Iminonjana Yabalandeli
Ukuhlolwa kokubukeka: ama-flakes amancane nensimbi noma izinsimbi ezingezona zensimbi nezensimbi zifakwa ama-welding, kanti ama-flakes amancane ayahluzwa ngaphansi kwesenzo samandla angaphandle. Ngemuva kokuxebuka, indawo yokusakaza iyakhanya kanti ezinye ziyimpunga emnyama.
Izizathu zingokulandelayo:
- 1) Kukhona izinsalela zensimbi noma ezingezona ezensimbi ebusweni bomgodi wokuphonsa
- 2) Lapho uthela, ukungcola kuqala kulethwa futhi kunamathiselwe ebusweni bomgodi
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Ngaphambi kokuphonsa ukufa, igumbi lokucindezela umgodi kanye nohlelo lokuthela kufanele kuhlanzwe ukuze kususwe abalandeli bensimbi noma okungebona abensimbi
- 2) Hlanza i-alloy cast
- 3) Khetha upende ofanele, futhi ukumboza kufanele kube
Ukubeka (Ukuncinza Nokuxebula)
Ukuhlola okubonakalayo noma ukuhlolwa kokulimala: Kunezingqimba ezisobala zensimbi engxenyeni yokulingisa.
Izizathu zingokulandelayo:
- 1) Isikhunta asiqinile ngokwanele. Ngesikhathi senqubo yokugcwalisa insimbi engamanzi, isifanekiso sizonyakaza
- 2) I-punch ibonakala ikhasa ngesikhathi senqubo yokujova
- 3) Idizayini engalungile yohlelo lomgijimi
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Qinisa ukuqina kwesikhunta bese uqinisa izingxenye zesikhunta ukuze uzenze zizinze
- 2) Lungisa ukubambisana kwesibhakela somjovo negumbi lengcindezi ukuqeda lo mkhuba wokukhasa
- 3) Dizayina ngokufanele umgijimi wangaphakathi
Ukungqubuzana Nokususwa Kwempahla
Ukuhlola okubonakalayo: Ubuso bengxenye yokulingisa inezindawo ezimbi ezindaweni ezithile.
Izizathu zingokulandelayo:
- 1) Isikhundla esingalungile, ukuqondiswa nokuma komgijimi wangaphakathi obangelwe yisikhunta sokufa (isikhunta)
- 2) Ukupholisa okunganele kwensimbi encibilikisiwe kumgijimi wangaphakathi obangelwa izimo zokuphonsa
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Ukwenza ngcono ukuma nokuqondiswa kwesipringi lapho kungalungile ukuthulula khona
- 2) Thuthukisa izimo zokupholisa, ikakhulukazi izindawo lapho insimbi encibilikisiwe ihlaselwe ngodlame
- 3) Faka upende engxenyeni evundlisiwe
- 4) Lungisa izinga lokugeleza kuketshezi lwe-alloy ukuvimbela i-cavitation
- 5) Susa abalandeli be-alloy ku-isikhunta (isikhunta)
Ukuguguleka kwenhlabathi
Ukuhlola okubonakalayo: Kunokugoba noma ukufaka embossing endaweni yangakini yokusakazwa kokufa.
Izizathu zingokulandelayo:
- 1) Ukusetha okungafanele kwesikhundla somgijimi wangaphakathi
- 2) Izimo ezipholile zokupholisa
Izixazululo nezindlela zokuvimbela yilezi:
- 1) Ubukhulu bomgijimi wangaphakathi kufanele bufanele
- 2) Shintsha indawo, indlela nokusetha umgijimi wangaphakathi
- 3) Qinisa ukupholisa kwezingxenye eziguguliwe.
Imifantu
Ukuhlola okubonakalayo: Faka ukusakaza kusixazululo se-alkaline, imifantu ayimpunga emnyama. Ukubhujiswa nokuqhekeka kwe-matrix yensimbi kuqondile noma ku-wavy, ngemigqa emincane futhi emide, enokuthambekela kokuthuthuka ngaphansi kwesenzo samandla angaphandle.
Izimbangela zokuqhekeka ku-aluminium alloy castings:
- 1) Okuqukethwe yensimbi ku-alloy kuphakeme kakhulu noma okuqukethwe kwe-silicon kuphansi kakhulu; okuqukethwe ukungcola okuyingozi ku-alloy kuphakeme kakhulu, okunciphisa ubuningi be-alloy; okuqukethwe i-zinc noma ithusi ku-aluminium-silicon alloy, i-aluminium-silicon-copper alloy iphezulu kakhulu; okuqukethwe kwe-aluminium-magnesium alloy kuphakeme kakhulu I-magnesium eningi kakhulu
- 2) Isikhathi sokugcinwa kwesikhunta sifushane kakhulu, futhi isikhathi sokubamba ingcindezi sifushane; ukushuba kodonga lokusakaza kunezinguquko ezinqala
- 3) Amandla okuqinisa endawo makhulu kakhulu, futhi amandla awalingani lapho ekhishwa
Izixazululo nezindlela zokuvimbela:
- 1) Lawula ngokufanele ukwakheka kwe-alloy. Kwezinye izimo: ama-aluminium pure ingots angafakwa ku-alloy ukunciphisa okuqukethwe kwe-magnesium ku-alloy; noma ama-aluminium-silicon master alloys angafakwa ku-alloy ukwandisa okuqukethwe kwe-silicon
- 2) Khulisa izinga lokushisa kwesikhunta (isikhunta); shintsha isakhiwo sokusakaza, lungisa indlela yokudonsa eyinhloko noma wenze amandla enduku yokudonsa ngokulinganayo
- 3) Khulisa i-engeli esalungiswa bese usebenzisa umenzeli oqinile wokukhishwa endaweni
- 4) Khulisa isikhathi sokugcina isikhunta futhi wandise isikhathi sokubamba ingcindezi
Sicela ugcine umthombo nekheli lale ndatshana ukuze uphinde uprintwe:Izixazululo Nezinyathelo Zokuvimbela I-Aluminium Die Casting 10 Amaphutha Amakhulu
UMinghe Inkampani yeDie Casting anikezelwe ekukhiqizeni nasekuhlinzekeni ikhwalithi nokusebenza okuphezulu Izingxenye Zokulingisa (izingxenye zensimbi zensimbi zokufa zisebenza ikakhulukazi zibandakanya I-Thin-Wall Die Casting,I-Hot Chamber Die Casting,Cold Chamber die Casting), Insizakalo Eyindilinga (Insiza Yokulingisa,ICnc Machining,Ukwenza Okubandayo, Surface Treatment) .Noma ikuphi ukusakazwa kwe-Aluminium die, i-magnesium noma i-Zamak / zinc die casting nezinye izidingo zokuphosa zamukelekile ukuxhumana nathi.
Ngaphansi kokulawulwa kwe-ISO9001 ne-TS 16949, Zonke izinqubo zenziwa ngamakhulu emishini esezingeni eliphakeme yokufa, imishini ye-5-axis, nezinye izikhungo, ezisukela kuma-blasters kuya kumishini yokuwasha ye-Ultra Sonic.Minghe akagcinanga ngemishini esezingeni eliphezulu kepha futhi unobuchwepheshe iqembu lonjiniyela abanolwazi, ama-opharetha nabahloli ukwenza ukwakheka kwekhasimende kugcwaliseke.
Umenzi wenkontileka yokufa kwabasikiwe. Amandla afaka izingxenye ezibandayo ze-aluminium die casting ezivela ku-0.15 lbs. kuye ku-6 lbs., Ukusetha ushintsho olusheshayo, nemishini. Izinsizakalo ezingezwe ngenani zifaka phakathi ukupholisha, ukudlidliza, ukuphazamisa, ukuqhumisa ngokudubula, ukupenda, ukuhlobisa, ukumboza, ukuhlangana nokusetshenziswa kwamathuluzi. Izinto zokusebenza ezisetshenzisiwe zifaka ama-alloys afana no-360, 380, 383, no-413.
I-Zinc die casting design usizo / izinsizakalo zobunjiniyela ezihambisanayo. Umenzi wangokwezifiso we-precision zinc die castings. Ukusakazwa okuncane, ukukhishwa kwengcindezi ephezulu, ukusikeka kwesikhunta esiningi, ukujikijelwa kwesikhunta okuvamile, ukufefa kwamayunithi kanye nokuzimela okuzimele kanye nokuvalwa okuvaliwe komgodi kungenziwa. Ama-Castings angenziwa ngobude nobubanzi obufinyelela ku-24 in. Ku +/- 0.0005 in. Ukubekezelelana.
I-ISO 9001: Umkhiqizi oqinisekisiwe ka-2015 we-die cast magnesium, Amandla afaka i-high-pressure magnesium die casting up to 200 ton chamber hot & 3000 ton cold chamber, designing designing, polishing, molding, machining, powder & liquid paint, QA full with CMM amakhono , inhlangano, ukupakisha nokulethwa.
Kuqinisekiswe i-ITAF16949. Insiza Eyengeziwe Yokulingisa Faka ukukhipha utshalomali,ukuphonsa kwesihlabathi,Ukuphonswa kwamandla, Lost Foam Ekubunjweni,I-Centrifugal Casting,Ukuphoswa Kokuqothula,Permanent Isikhunta Ukulingisa, Amakhono afaka i-EDI, usizo lobunjiniyela, ukumodeliswa okuqinile nokucutshungulwa kwesibili.
Izimboni Zokulingisa Izingxenye Zamacala Ezifundo Zezimoto: Izimoto, Amabhayisikili, Izindiza, Izinsimbi Zomculo, I-Watercraft, Amadivayisi we-Optical, Izinzwa, Amamodeli, Amadivayisi we-elekthronikhi, Ukuvaleka, Amawashi, Imishini, Izinjini, Ifenisha, Ubucwebe, AmaJig, Telecom, Ukukhanyisa, Amadivayisi Wezokwelapha, amadivayisi wezithombe, Amarobhothi, okubaziwe, okokusebenza komsindo, okwezemidlalo, i-Tooling, Amathoyizi nokuningi.
Yini esingakusiza ukuthi uyenze ngokulandelayo?
∇ Iya ekhasini eliyisiqalo For I-Die Casting China
→Izingxenye Zokusakaza-Thola esikwenzile.
→ Izeluleko Ezilinganisiwe Mayelana Izinsizakalo Zokufa Zokusakaza
By Umkhiqizi weMinghe Die Casting | Izigaba: Izindatshana Eziwusizo |Material Omaka: I-Aluminium Casting, Zinc Ukulingisa, Ukulingiswa kweMagnesium, I-Titanium Casting, Insimbi Engagqwali, Brass Ekubunjweni,Ukulingiswa kweBronze,Isakaza ividiyo,Umlando wenkampani,I-Aluminium Die Casting | Amazwana Off